Corrugated base paper (corrugating medium) is the fluted core that gives corrugated boxes their stacking and compression strength, and its quality in China is governed by the national standard GB/T 13023-2008. National standard testing verifies grammage, moisture, Concora flat crush strength (CMT), short-span compression and other key indicators using standardized laboratory methods such as GB/T 451.2, GB/T 462 and GB/T 2679.3. This guide explains the scope of testing, sampling and conditioning requirements, test items, methods, and typical applications for manufacturers, converters and buyers.
Technical Overview
Corrugated base paper, also known as corrugating medium, is the fluted sheet bonded between linerboards to form corrugated board. Its compression performance directly determines the edge crush strength, stacking strength and transport safety of finished corrugated packaging. In China, product quality is governed by the national standard GB/T 13023-2008 (Corrugating medium), which classifies the product into quality grades and specifies requirements for grammage, tightness, moisture, Concora flat crush strength (CMT), appearance and related indicators.
The standard applies to corrugating medium produced from recycled or virgin fibers and supplied in rolls or sheets. All physical test methods are supported by companion national standards that are harmonized with corresponding ISO methods, which ensures that results are technically equivalent and comparable in international trade. Accredited third-party laboratories, mill quality-control departments and converter incoming-inspection teams routinely perform this suite of tests.
Testing Samples
Product Grades and Specifications
- Quality grades: superior grade, first grade and qualified grade, each with progressively higher minimum strength requirements.
- Nominal grammage series: commonly 80, 90, 100, 110, 120, 140, 160, 180 and 200 g/m².
- Product form: rolls or flat sheets; the submitted sample must be representative of the entire production lot and free from transport damage.
Sampling Requirements
Sampling is performed in accordance with GB/T 10342 (Sampling of paper and board). Samples are taken at defined positions across the reel width and along the machine direction so that both cross-direction and machine-direction properties are represented. Samples must be protected from moisture, crushing and contamination during packaging and transport, because edge damage and humidity changes can invalidate strength results.
Sample Conditioning
Before physical testing, specimens are conditioned in the standard atmosphere defined by GB/T 10739, i.e. (23 ± 1) °C and (50 ± 2) % relative humidity, until moisture equilibrium is reached. Conditioning is essential because paper strength is highly sensitive to ambient humidity, and unconditioned specimens can produce results that deviate significantly from the true values.
Testing Items
A typical national-standard test program for corrugating medium includes the following items:
- Quantitative (grammage) and grammage deviation — GB/T 451.2.
- Thickness and tightness (apparent density) — GB/T 451.3.
- Moisture content at delivery — GB/T 462.
- Concora flat crush strength, CMT0 and CMT30 — GB/T 2679.3.
- Short-span compression strength (SCT) — GB/T 2679.10.
- Bursting strength — GB/T 454 or GB/T 1539.
- Tensile strength and breaking length — GB/T 12914.
- Water absorption (Cobb value) — GB/T 1540.
- Ash content — GB/T 742.
- pH value of the aqueous extract — GB/T 1545.
- Appearance: wrinkles, holes, dirt spots, roll damage and splice quality.
Among these, CMT30 is the defining performance index for corrugating medium. It measures the ability of a laboratory-fluted specimen to resist flat crushing after 30 minutes of recovery time, simulating the flute strength retained after storage and converting. Higher grammage grades are required to achieve proportionally higher CMT values, and the minimum limits differ for each quality grade.
Testing Methods
Concora Flat Crush Test (CMT)
A specimen strip is fluted on a laboratory fluting device under a defined pressure and secured with adhesive tape to hold the flute geometry. The fluted specimen is then placed between the parallel platens of a compression tester and crushed flatwise at the specified speed. For CMT30, the specimen is conditioned for 30 minutes after fluting before testing; CMT0 denotes immediate testing after fluting and is sometimes used for internal process control. The maximum force, expressed in newtons, is reported.
Grammage, Thickness and Tightness
Grammage is determined by weighing conditioned specimens of accurately known area on a calibrated balance and expressing the result in g/m². Thickness is measured with a dead-weight micrometer under a standardized contact pressure, and tightness (apparent density) is calculated as grammage divided by thickness. Low tightness often indicates a bulky but weak fiber network that will deliver poor compression performance.
Moisture Content Determination
Moisture is determined by drying representative specimens in an oven at (105 ± 2) °C to constant mass, with the moisture content calculated from the mass loss. The national standard specifies delivery moisture limits within a controlled range, because excessive moisture softens the fiber network and reduces flute strength, while overly dry paper becomes brittle and prone to cracking on the corrugator.
Strength Testing (Burst, Tensile and SCT)
Bursting strength is measured by clamping the specimen over a diaphragm and applying increasing hydraulic pressure until rupture. Tensile strength and breaking length are measured on a tensile tester at a constant rate of elongation. Short-span compression strength (SCT) compresses a very short, guided specimen length and correlates closely with the final edge crush performance of the finished corrugated board, making it an increasingly important supplementary index.
Data Processing and Conformity Judgment
Measured values are statistically processed according to the rules of each method standard, and results are rounded and reported as required by GB/T 13023. If any indicator falls outside the limit for the declared grade, the standard's retest provisions apply, typically requiring duplicate specimens from the original sample. A lot is judged conforming only when all specified items, including appearance, meet the requirements of the declared grade.
Applications
National standard testing of corrugated base paper supports the entire corrugated packaging supply chain:
- Incoming inspection at corrugated box plants to verify that purchased medium meets the contracted grade before production.
- Internal quality control and grade determination at paper mills, including release testing of production batches.
- Supplier qualification, audits and comparative benchmarking of competing furnish recipes or recycled fiber sources.
- Trade settlement and arbitration when disputes arise over delivered quality between buyers and sellers.
- Research and development of recycled fiber formulations, sizing strategies and energy-optimized refining.
- Compliance documentation for customer audits, tender submissions and export shipments where GB-based certificates are requested.
FAQ
Q: Which national standard applies to corrugated base paper?
A: GB/T 13023-2008 (Corrugating medium) is the applicable national standard. Linerboard (box board), the flat facing layer, is governed separately by GB/T 13024, and the two standards are often tested together for a complete board furnish evaluation.
Q: What is the difference between CMT0 and CMT30?
A: CMT0 is measured immediately after fluting, while CMT30 is measured after the fluted specimen has recovered for 30 minutes. The 30-minute value is the contractual index in the national standard because it better reflects the flute strength retained in real converting and storage conditions.
Q: How much sample is needed for a full test program?
A: Laboratories typically request several full-width sheets or a roll section of at least 0.5 meter in length, packaged flat and moisture-protected, so that sufficient specimens can be cut for every test item and any required retests.
Q: Is GB/T 13023 a mandatory standard?
A: GB/T 13023 is a recommended national standard, so its use is voluntary in principle; however, it becomes contractually binding once referenced in purchase agreements, product labels or tender specifications.
Q: How long does testing take?
A: Including sample conditioning at the standard atmosphere, a complete test program is normally completed within five to seven working days, with express services available for urgent production decisions.
Q: Which properties matter most for final box strength?
A: CMT and SCT of the medium, combined with the ring-type compression behavior of the liners, are the dominant contributors to board edge crush strength and warehouse stacking performance, which is why they receive the closest attention in national standard testing.
Why Choose ZKGX?
- State-of-the-art analytical equipment
- Highly qualified scientific team
- Fast turnaround time
- Competitive pricing